US20050082172A1 - Copper replenishment for copper plating with insoluble anode - Google Patents
Copper replenishment for copper plating with insoluble anode Download PDFInfo
- Publication number
- US20050082172A1 US20050082172A1 US10/690,408 US69040803A US2005082172A1 US 20050082172 A1 US20050082172 A1 US 20050082172A1 US 69040803 A US69040803 A US 69040803A US 2005082172 A1 US2005082172 A1 US 2005082172A1
- Authority
- US
- United States
- Prior art keywords
- copper
- plating solution
- anolyte
- chemical reagent
- tank
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Abandoned
Abstract
In one embodiment, the present invention generally provides an apparatus and method for dispersing a chemical reagent into a plating solution. The apparatus generally includes a tank for containing the plating solution and a horizontal vessel in fluid communication with the tank, wherein the horizontal vessel has an input and an output. The apparatus further includes at least one shelf contained inside the horizontal vessel, wherein the at least one shelf extends between the input and the output and the chemical reagent rests on the at least one shelf. In another embodiment, the present invention generally provides an apparatus for dispersing a chemical reagent to a plating solution comprising a tank for containing the plating solution and a vertical vessel in fluid communication with the tank. A lower portion of the vertical vessel includes an inlet and an injector port and an upper portion of the vertical vessel includes an outlet and a manifold. The chemical reagent is positioned between the inlet and the outlet.
Description
- 1. Field of the Invention
- Embodiments of the invention generally relate to a metal plating apparatus and process, namely for the replenishment of chemical components used to electroplate copper.
- 2. Description of the Related Art
- Semiconductor substrates can be plated with copper by electroplating or electroless plating processes. During the electroplating, an anode is usually placed into an electrolyte solution and the substrate is conductively coupled to a cathode. As current flows, dissolved copper ions from the electrolyte solution are reduced and plated (or deposited) on the surface of the substrate as copper metal. Traditionally, the anode is made from consumable copper metal and is continuously oxidized to provide copper ions to the plating process. Due to the consumption of the copper anode, the dimension of the copper anode is changed. Therefore the directional electrical fields produced by the anode also change accordingly. This alteration in the electric field presents a challenge to precisely control the electroplating process, especially within vias with high aspect ratios.
- Another electroplating process utilizes an inert or stable anode in place of a consumable anode. The use of an inert anode provides excellent control for precision plating since the anode is not consumed during the plating process. However, the inert anode does not supply a source of copper into the electrolyte solution. As the copper ions are reduced and plated from the electrolyte solution to the substrate surface, the copper ion concentration in the electrolyte solution is diminished. Therefore, as the plating process progresses, a copper source, namely copper ions, must be added to the electrolyte solution in order to continue the plating process. Copper sources are generally chosen from a variety of copper salts that include copper sulfate, copper hydroxide, copper oxide and copper phosphate.
- U.S. Pat. No. 5,516,414 teaches a method to maintain an alkaline copper plating solution with a desired concentration of copper ions and hydroxide ions. The '414 patent discloses adding copper hydroxide powder from a conduit to an alkaline, pyrophosphate solution in a dissolving tank. Once the solution has been heated and agitated to insure that the copper hydroxide has been dissolved, the pyrophosphate solution is transferred via a pump to the plating solution. The plating solution is monitored with a meter and maintained with a basic pH between 7 and 10 by adding the alkaline, pyrophosphate solution. Though the addition of copper hydroxide powder is adequate in the realm of electroplating wires, this technique is unacceptable in a clean environment, such as a semiconductor fabrication room equipped to plate substrates. The dumping of a powdery precursor into a solution would present contamination issues for semiconductor processing in a cleanroom environment.
- U.S. Pat. No. 5,997,712 realizes the shortcomings of the '414 patent as applied to a cleanroom. The '712 patent avoids dumping the powdery precursor and teaches a method to replenish copper ions in a plating solution with the apparatus depicted in
FIG. 1A . The anolyte flows from the top ofcanister 2, through aporous cartridge 4 and into ahollow cavity 6 before flowing out the bottom ofcanister 2. Thecartridge 4 includes a filter element that encompasses the powdery copper source. Therefore, the anolyte flows through thecanister 2 and is enriched by copper ions via absorbing the copper source. - However, as illustrated in
FIG. 1B , the anolyte can flow intocartridge 4 and form different phases of anolyte/copper source. Thedepleted anolyte 8 enters thecartridge 4 from above and flows downwardly to form asuspension 9 of anolyte/copper source. As thesuspension 9 flows towards the bottom of thecartridge 4, the suspension densifies, forming aviscous cake 10 at the bottom of thecartridge 4. Throughout the formation ofcake 10, the flow of anolyte lessens and copper ions cease to be consistently replenished in the anolyte. Therefore, longer plate times reduce substrate throughput with this decrease of the copper concentration. Also, in the case when copper hydroxide is used as a copper source, the reduction in the hydroxyl ion addition lowers the pH of the anolyte. - Therefore, there is a need for an apparatus and method to replenish chemical compounds within an electrolyte solution in a consistent and reliable manner.
- In one embodiment, the invention generally provides an apparatus for dispersing chemical reagents to a plating solution including a tank for containing the plating solution and a cartridge in fluid communication with the tank, wherein the cartridge has an input and an output. The apparatus further includes at least one shelf contained inside the cartridge. The at least one shelf may be impermeable and may extend between the input and the output such that the chemical reagent rests on the at least one shelf.
- In another embodiment, the invention generally provides an apparatus for dispersing a chemical reagent to a plating solution comprising a tank for containing the plating solution and a vertical cartridge in fluid communication with the tank. A lower portion of the vertical cartridge includes an inlet and an injector port and an upper portion of the vertical cartridge includes an outlet and a manifold. The chemical reagent is positioned between the inlet and the outlet.
- In another embodiment, the invention generally provides a method for dispersing a chemical reagent to a plating solution including flowing the plating solution from a tank through an input of a cartridge, wherein the cartridge comprises a chemical reagent disposed on at least one shelf. The plating solution flows across the chemical reagent to enrich the plating solution with the chemical reagent, whereas the chemical agent is dissolved or suspended within the plating solution. The enriched plating solution flows from the cartridge through an output to the tank.
- In another embodiment, the invention generally provides a method for monitoring and controlling a pH setting of a plating solution in a tank including determining a pH of the plating solution with a pH meter, transferring an aliquot of the plating solution to a vessel and pressurizing the vessel with a gas to transfer the aliquot to a cartridge. The cartridge includes an injector, a chemical reagent and a manifold. The aliquot passes through the injector, which enriches the aliquot with a portion of the chemical reagent and the enriched aliquot transfers through the manifold to the plating solution in the tank. A second pH of the plating solution is determined with the pH meter and compared with the pH setting. Enriched aliquots are transferred repeatedly to the plating solution until the second pH is equivalent to the pH setting.
- So that the manner in which the above recited features of the present invention can be understood in detail, a more particular description of the invention, briefly summarized above, may be had by reference to embodiments, some of which are illustrated in the appended drawings. It is to be noted, however, that the appended drawings illustrate only typical embodiments of this invention and are therefore not to be considered limiting of its scope, for the invention may admit to other equally effective embodiments.
- FIGS. 1A-B show a cartridge inside a canister as used in the related art;
-
FIG. 2 shows a flow diagram for a two-sectional electrochemical cell with catolyte and anolyte; -
FIG. 3 shows a longitude sectional view of a cartridge with horizontal shelves; - FIGS. 4A-C show cross-sectional views of cartridges with a variety of shelves;
- FIGS. 5A-C show cartridge placements into an anolyte loop;
-
FIG. 6A shows a vertical sectional view of a cartridge with a bottom injector; -
FIG. 6B shows a fragmentary vertical sectional view of a portion of the embodiment ofFIG. 6A ; -
FIG. 7 shows a schematic diagram of a plating system incorporating one embodiment of a cartridge with a bottom injector; -
FIG. 8 is a diagram illustrating the timing sequence of valve operation during a plating process; -
FIG. 9 shows another embodiment of a cartridge with a bottom injector incorporated into a plating system; and - FIGS. 10A-B show embodiments of injector systems including rotatable cups.
- The present invention comprises apparatuses and methods to replenish chemical compounds in plating solutions in a consistent and reliable manner. The present invention overcomes the shortcomings of the related art as described in the background and illustrated in
FIG. 1 , mainly, by not blocking anolyte flow with cake formations. Therefore, by utilizing the various embodiments of the apparatuses and methods of the present invention, each substrate experiences more consistent plating times and anolyte chemical concentrations. - Embodiments of the present invention are useful in a variety of plating systems, including electroplating and electroless plating systems. Further, various embodiments are also applicable to electroplating with soluble anodes and with insoluble anodes.
FIG. 2 shows a schematic arrangement of an electroplating system with acell 11 containing aninsoluble anode 12. Theinsoluble anode 12 is made from relatively inert materials, such as platinum, titanium, titanium with a Pt-coating, palladium, nickel, stainless steel and/or carbon. The material of theinsoluble anode 12 is generally configured to withstand the various process conditions involved while plating to a wafer orsubstrate 14. Process conditions may have acidic or basic pH, oxidative/reductive potentials and an assortment of chemical compounds throughout the solution. In one embodiment, theinsoluble anode 12 endures process conditions such as acidic plating solutions and an oxidative potential. Thesubstrate 14 is attached to the cathode 13, usually by a contact ring, pins, and the like (not pictured). - The
insoluble anode 12 and the cathode 13 are separated by amembrane 16 extending throughcell 11. Themembrane 16 is an electroconductive membrane, such as an ion-exchange membrane, nano-filtration membrane, ultra-filtration membrane and others known in the art. The portion of thecell 11 containing the cathode 13 is in fluid communication with thecatolyte tank 17 to recirculate the catolyte within. The catolyte is a mixture of compounds that may include, for copper plating, sulfuric copper plating electrolyte or pyrophosphoric copper plating electrolyte. A sulfuric copper plating electrolyte will generally include a mixture of copper sulfate, sulfuric acid and various organic and inorganic additives including suppressors, accelerators, levelers and brighteners. Catolyte may pass through adiffuser 15 and be more evenly distributed while flowing to thesubstrate 14. - The portion of the
cell 11 containing theinsoluble anode 12 is in fluid communication with theanolyte tank 18 and recirculates the anolyte within. For copper plating, the anolyte is a solution containing copper ions, often derived from dissolved copper salts, such as copper sulfate. Other copper ion sources include copper hydroxide, copper carbonate, copper oxide and copper phosphate. - Under copper plating electrolysis, the half reaction in scheme (i) occurs on the insoluble anode 12:
H2O→2H++2e−+½O2(g), (i)
while Cu2+ ions migrate through themembrane 16 from the anolyte to the catolyte and are reduced according to the half reaction shown in scheme (ii):
Cu2++(SO4)2−+2e−→Cu0+(SO4)2−. (ii)
The combined half reactions are represented in reaction scheme (iii):
CuSO4+H2O→Cu0+H2SO4+½O2(g) (iii)
Therefore, as the electroplating process proceeds, the anolyte becomes depleted of copper ions due to the precipitation of metallic copper as well as more acidic due to the production of sulfuric acid. Also, water is consumed making the electrolyte more concentrated. - The sulfuric acid formed in the anolyte penetrates through the
membrane 16 and contaminates the catolyte. The sulfuric acid lowers the pH of the catolyte. More acidic catolyte is not desirable because the membrane loses ion selectivity between protons and copper ions. The lost of the membrane selectivity permits protons to compete with copper ions while penetrating the membrane, therefore, unbalancing the catolyte chemical concentration. To prevent the lowering of the pH of the catolyte, an alkaline compound is added. Copper hydroxide consists of a copper ion source as well as a hydroxyl source and will neutralize formed sulfuric acid, as shown by the reaction scheme (iv):
Cu2++2(OH)−+H2SO4→CuSO4+2H2O. (iv)
Therefore, schemes (iii) and (iv) are combined and the proportional amount of copper hydroxide is added to the anolyte. The summed reaction is depicted in scheme (v), namely copper is consistently deposited while water and oxygen are formed as byproducts, such as:
Cu(OH)2→Cu0+H2O+½O2(g). (v) -
FIG. 3 shows a longitudinal sectional view of an embodiment of acartridge system 20 including acartridge 22 containing one embodiment ofshelves 24 of the invention. Theshelves 24 are vertically spaced apart and extend longitudinally betweeninput 32 andoutput 34. Theshelves 24 may number in a range from about 1 to about 50, though preferably from about 2 to about 10.FIGS. 3 and 4 A illustrate four horizontal substantially flat top shelves. Thecartridge 22 and theshelves 24 may be made from an assortment of materials, such as plastics or metals, including stainless steel, aluminum, titanium, nickel-coated steel and various alloys, amongst others. -
Chemical reagents 26 are distributed across each of theshelves 24. The chemical reagents are exposed to plating solution 28 (depicted with arrows) flowing through thecartridge 22. Theplating solution 28 enters the cartridge at least partially depleted of various chemical components, but is enriched by flowing over thechemical reagents 26 contained within thecartridge 22. The enriching process includes the dissolving and/or suspending ofchemical reagents 26 within theplating solution 28. Thechemical reagents 26 usually have a solid state of matter (e.g., powder, pellets, crystalline), but could also be a viscous liquid or a suspension. Therefore, enriched platingsolution 29 emerges from theoutput 34. A progressive and consistent transformation or enrichment of the plating solution occurs as platingsolution 28 flows acrosschemical reagents 26. In one example, theshelves 24 are impermeable to liquids (e.g., metal plate with no holes or no porosity), so theplating solution 28 passes along and not through theshelves 24. In another example, theshelves 24 are permeable to liquids, such as ceramic or mesh, so theplating solution 28 passes along and/or through theshelves 24. -
Chemical reagents 26 are compounds or mixtures of compounds selected for the process requirements of the plating solution. Plating solutions include electroless plating solutions and electroplating solutions, wherein the latter is usually the anolyte or the catolyte. Electroplating systems are utilized to deposit materials such as copper, zinc, cadmium, nickel and other metals. In one preferred embodiment, the plating solution is an anolyte within an electroplating system used to plate copper. -
Chemical reagents 26 useful for copper ion replenishment in a plating solution include copper hydroxide, copper oxide, copper carbonate, copper sulfate and copper phosphate and combinations thereof, preferably copper hydroxide. Generally, plating solutions, enriched or depleted, have a copper ion concentration in a range from about 5 g/L to about 70 g/L. -
Chemical reagents 26 are also used to replenish plating solutions of other depleted compounds and ions. In one embodiment, chemical reagents are used to control the pH of the plating solution. The pH of the solution can be raised or lowered by adding a basic or acidic compound, respectively.Chemical reagents 26 for replenishing hydroxyl ions to increase the pH include copper hydroxide, ammonium salts, sodium hydroxide, potassium hydroxide, lithium hydroxide, cesium hydroxide, magnesium hydroxide, calcium hydroxide, amongst others, and combinations thereof. Therefore, in one embodiment, copper hydroxide is used to replenish copper ions and hydroxyl ions. -
Porous material 25 is optionally placed at either or both ends of thecartridge 22 and include porous plastics, metals, ceramics, filters, frits, membranes, wool (e.g., glass or metal), packed inert media (e.g., silica or alumina) and the like. Generally, the porous material has pores that are penetrable for enriched plating solution (suspensions), but preventschemical reagents 26 from uncontrollably passing through thecartridge 22. The porous material has pores with a diameter in the range from about 10 μm to about 2,000 μm. - FIGS. 4A-C show cross-sectional views of
cartridge system 20 with a variety of geometries for cartridges and shelves.FIG. 4A shows the fourflat shelves 24 ofFIG. 3 as described above.FIG. 4B shows shelves withlongitudinal grooves 36. Thegrooves 36 further segregate thechemical reagents 26 into various rows running along each shelf.FIG. 4C shows acylindrical cartridge 37 containingtubular shelves 38.Tubular shelves 38 also holdchemical reagents 26 in segregated rows. The shelves distribute (i.e., provide more surface area)chemical reagents 26. Time exposure between the plating solution and the chemical reagent varies the degree of enrichment the plating solution endures. Therefore, the flow of the plating solution throughcartridge 22 varies in a range from about 0.5 L/min to about 10 L/min, depending on the bath volume and performance. - The flow of the plating solution is maintained due to part of
headspace 30 provided above the top surface of thechemical reagents 26. Generally,headspace 30 has a height in the range from about 1 cm to about 50 cm, preferably from about 5 cm to about 30 cm.Headspace 30 changes throughout the process with respect to time, since thechemical reagents 26 are consumed by the plating solution and the height of headspace increases. Also,headspace 30 changes throughout the process with respect to certain segments along the shelves. Besides consumption,chemical reagents 26 also migrate and erode along the shelves. - In several examples, as depicted in FIGS. 5A-C,
cartridge system 20 is placed into anolyte loops with various configurations. In one embodiment,FIG. 5A showscartridge system 20 placed into a single anolyte loop. As anolyte requires replenishment of chemical reagents (e.g., Cu2+ or OH−), pump 120 draws depleted anolyte from theanolyte tank 110. Withcontrol valve 130 open, pump 120 pushes the depleted anolyte throughcartridge system 20. The anolyte emerges from thecartridge system 20 enriched with the specific chemical reagents required for the plating process (e.g., Cu(OH)2). Upon exiting thecartridge system 20, anolyte flows to theelectroplating cell 100, where the plating process commences, forming depleted anolyte, which is transferred back to theanolyte tank 110. This cycle resumes as the anolyte is recirculated throughout the anolyte loop. - In another embodiment,
FIG. 5B showscartridge system 20 placed into an anolyte loop also including a bypass line. The bypass line is useful when the anolyte is only partially depleted of the necessary chemical reagents. Though depleted anolyte will contain some essential chemical reagents, the concentration of the reagents is too low and affects the plating process. However, partially depleted anolyte is suited to be recirculated and used in the electroplating process prior to being enriched bycartridge system 20. Depleted or partially depleted anolyte is determined per process parameters. As anolyte requires replenishment of chemical reagents (e.g., Cu2+ or OH−), pump 120 draws depleted anolyte from theanolyte tank 110. Withcontrol valve 130 open andcontrol valve 135 closed, pump 120 pushes the depleted anolyte throughcartridge system 20. The anolyte emerges from thecartridge system 20 enriched with the specific chemical reagents required for the plating process (e.g., Cu(OH)2). Upon exiting thecartridge system 20, anolyte flows to theelectroplating cell 100. However, withcontrol valve 130 closed andcontrol valve 135 opened, pump 120 pushes the partially depleted anolyte through a bypass around thecartridge system 20 and directly to theelectroplating cell 100. Upon the commencement of the plating process, depleted anolyte is transferred back to theanolyte tank 110. This cycle resumes as the anolyte is recirculated throughout the anolyte loop. - The anolyte cycle system depicted in
FIG. 5B has an advantage over the system depicted inFIG. 5A due to the cartridge bypass line, namely, more control of the supplemental chemical reagent addition. Since the system ofFIG. 5B has the bypass line, anolyte is recirculated with the option to pass throughcartridge system 20. For any of the anolyte loops depicted in FIGS. 5A-C, the capacity ofanolyte tank 110 can be increased to slow the anolyte dilution from the addition of depleted anolyte coming fromcell 100. - The system depicted in
FIG. 5C includes several anolyte loops linked together via theanolyte tank 110. One loop includes theelectroplating cell 100 in fluid communication with theanolyte tank 110.Pump 120 circulates the anolyte within this loop. However, an auxiliary loop is also linked with theanolyte tank 110. The auxiliary loop includes thecartridge system 20 connected to acontrol valve 134 and apump 125. In one aspect, pump 125 is a high-pressure pump. Also incorporated to the auxiliary loop is a bypass line managed bycontrol valve 132. Therefore in one aspect, withcontrol valve 134 opened andcontrol valve 132 closed, anolyte can be circulated between theanolyte tank 110 andcartridge system 20 to be enriched with chemical reagents, while the anolyte is circulated between theanolyte tank 110 and theelectroplating cell 100. In another aspect,control valve 134 is closed whilecontrol valve 132 is opened andcartridge system 20 does not replenish the supplemental chemical reagents to the system. - In another embodiment, FIGS. 6A-
B show cartridge 40 as a vertical vessel in which a lower portion of the interior of the vessel expands upwardly to form an inverted conical bottom 42. Thecartridge 40 includes top 39 as a portion ofhousing 41, both made from an assortment of materials, such as plastics or metals, including stainless steel, aluminum, titanium, nickel-coated steel, various alloys amongst others. - At the base of the conical bottom 42, an
injector 43 is positioned in a vertical arrangement. The conical bottom 42 collects the settlingchemical reagents 26 by gravitational forces. This settling process maintains thechemical reagents 26 in contact with theinjector 43. The injector has aninput 45 that is in fluid communication with the electroplating system. Depletedelectrolyte 28 combined with or without gas (e.g., air) passes through theinput 45 and is introduced into thecartridge 40 through at least oneoutput 47 ofinjector 43. In one embodiment, there aremultiple outputs 47 in asingle injector 43. The orifice that provides theoutput 47 generally has a diameter in the range from about 0.1 mm to about 1 mm. As depicted inFIG. 6B , outputs 47 are less than normal (i.e., <90°) relative to the plane of the axis of theconical bottom 42. That is, theoutputs 47 generally point downward, towards the conical bottom 42 and extend through thesides 48 ofinjector 43. However, in one embodiment (not shown), the channels are normal or pointing upward, but have an optional flap in order to keep chemical reagent from descending into the outputs. - Plating solution or electrolyte is administered into the
cartridge 40 through theinjector 43.Chemical reagents 26 are disposed within thecartridge 40, so the electrolyte travels through thechemical reagents 26 and into aheadspace 49. An under pressure (e.g., vacuum system) and/or an over pressure (e.g., compressed gas) is utilized to assist the migration of the electrolyte through thecartridge 40. The electrolyte becomes enriched with thechemical reagents 26, (i.e., dissolved or suspended) while passing through thecartridge 40. The enrichedelectrolyte 29 accumulates near or at theheadspace 49, and then proceeds to exit thecartridge 40 through the manifold 44. In one embodiment, theheadspace 49 has enrichedanolyte 29 as well as accumulatedgas 46 or air. The accumulatedgas 46 is bled from the headspace prior or during the flow of enrichedanolyte 29. In another embodiment, a porous material (not shown), such as sponges, porous plastics, metals, ceramics, filters, frits, membranes, wool (e.g., glass or metal), packed inert media (e.g., silica or alumina) and the alike is displaced below the manifold 44 to inhibit any large particulate ofchemical reagents 26 from leaving thecartridge 40. - In another embodiment,
FIG. 7 shows aplating system 50 that includes acartridge 40 of the invention. The enrichedelectrolyte 29 is added toanolyte tank 52, which is in fluid communication with anelectroplating cell 56 and pump 58 within an anolyte loop. Anolyte is depleted of reagent chemical (e.g., CU2+ and OH−) during the plating process within theelectroplating cell 56.Pump 58 drives the circulation of depleted anolyte to theanolyte tank 52 and enriched anolyte from theanolyte tank 52 to theelectroplating cell 56. - A
pH controller 54,pH sensor 57 and acomputer 55 monitor and regulate the pH of the anolyte within theanolyte tank 52. A pH controller may be selected from a variety of commercially available models, such as dTRANSpH 01 from JUMO Process Control Inc., DP24-E Process Meter from Omega, EMIT-pH from Pathfinder Instruments, and LED pH/ORP indicator/controller from Kemko Instruments. In one embodiment, the pH is maintained in the range from about 1.0 to about 5.0, preferably, from about 2.0 to about 4.0 and more preferably from about 2.8 to about 3.0. In another embodiment, the pH is maintained at less than 3.4 to prevent chemical precipitants (e.g., copper hydroxide) from forming and clouding the anolyte. - As the pH of the anolyte becomes too low, an aliquot of the anolyte is transferred from
anolyte tank 52 tocanister 53 via three-way valve 60. Generally, three-way valve 61 is positioned to pressurizeanolyte tank 52 with compressed gas (e.g., air) and three-way valve 60 is positioned as to accept the aliquot from theanolyte tank 52 to thecanister 53. Once the aliquot is transferred, then bothvalves way valve 61 is positioned to pressurize thecanister 53 containing the aliquot of the anolyte while three-way valve 60 is positioned to permit the flow of the aliquot into thecartridge 40 via theinjector 43. The enriched anolyte emerges from thecartridge 40 via themanifold 44 and into theanolyte tank 52. As the enriched anolyte combines with the depleted anolyte, acidic protons are neutralized by the incoming hydroxyl ions and copper ions become more concentrated. In practice, the concentration of the anolyte will not vary much since control of the replenishment is occurring real time. That is, whenvalves source 62, such as a tank or an in-house line and may include air, N2, Ar, He, H2 and combinations thereof. -
FIG. 8 is a diagram illustrating a timing sequence ofvalves plating system 50 depicted inFIG. 7 . The timing ofvalves pH controller 54 in combination with acomputer 55. Thevalves canister 53 intocartridge 40. The time t1 is slightly longer (e.g., about a second) than that required to push all of the anolyte fromcanister 53, so that a small amount of air also penetrates in to thecartridge 40. The air provides a thorough mixing of the chemical reagents with the anolyte and enriches the suspension (e.g., copper hydroxide) near the top of thecartridge 40 withinheadspace 49. This thorough mixing with the air and the conical shape of the bottom of the cartridge prevents cake formation. During time t2, compressed air is stopped by closingvalve 61 andcanister 53 is refilled with anolyte throughvalve 60. During t3, the anolyte is injected intocartridge 40 with the timing quick enough to prevent penetration of air into thecanister 53, about a second.Canister 53 is refilled with anolyte that is subsequently injected into thecartridge 40. Thereafter, an enriched anolyte is transferred from thecartridge 40 to theanolyte tank 52. This cycle continues until the pH reaches a higher limit (HL), then ceases until the pH of the anolyte within the anolyte tank reaches the LL. The overall sequence repeats during the electroplating process. - In another embodiment,
FIG. 9 shows aplating system 70 that includes acartridge 40. The enrichedelectrolyte 29 is added toanolyte tank 52, which is in fluid communication with anelectroplating cell 56 and pump 58 within an anolyte loop. Anolyte is depleted of reagent chemical (e.g., Cu2+ and OH−) during the plating process within theelectroplating cell 56.Pump 58 drives the circulation of depleted anolyte to theanolyte tank 52 and enriched anolyte from theanolyte tank 52 to theelectroplating cell 56. The depleted anolyte is temporally contained within asection 71 of theanolyte tank 52.Section 71 is separated bypartition 80 and will gather depleted anolyte as well as enriched anolyte, before flowing over into the main compartment ofanolyte tank 52. - A
pH controller 54,pH sensor 57 and acomputer 55 monitors and regulates the pH of the anolyte withinsection 71. In one embodiment, the pH is maintained in the range from about 1.0 to about 5.0, preferably, from about 2.0 to about 4.0 and more preferably from about 2.8 to about 3.0. In another embodiment, the pH is maintained at less than 3.4 to prevent chemical precipitants (e.g., copper hydroxide) from forming and clouding the anolyte. - As the pH of the anolyte becomes too low, an aliquot of the anolyte is transferred from
anolyte tank 52 tocanister 53 via two-way valve 76.Pump 58 helps push the anolyte tocanister 53. Once the aliquot is transferred, then two-way valve 72 is positioned to pressurize thecanister 53 containing the aliquot of the anolyte while two-way valve 78 is positioned to permit the flow of the aliquot into thecartridge 40. The enriched anolyte flows from thecartridge 40 tosection 71 of theanolyte tank 52. As the enriched anolyte combines with the depleted anolyte, acidic protons are neutralized by the incoming hydroxyl ions and copper ions become more concentrated. Two-way valve 74 is positioned open and gas flow agitates the enriched anolyte with the depleted with the flow of gas. In practice, the concentration of the anolyte will not vary much since the replenishment is occurring in real time. That is, whenvalves source 62, such as a tank or an in-house line and may include air, N2, Ar, He, H2 and combinations thereof. - In one embodiment depicted in
FIG. 10A ,injector system 82 includes aninjector 84 withoutput holes 85 and acup 86 with output holes 87.Cup 86 is rotatable as to line-up the output holes 85 with output holes 87. Once lined-up, anolyte will pass throughholes cartridge 40, output holes 85 and 87 are misaligned to turn off the excess ofchemical reagents 26 from escaping thecartridge 40.FIG. 10A illustratescup 86 disposed within theinjector 84, while in another embodiment,FIG. 10B shows aninjector 94 disposed within acup 96 as part ofinjector system 92. Also,injector 94 contains output holes 95 andcup 96 contains output holes 97. The output holes 85 and 87 generally point horizontal while the output holes 95 and 97 point in a downwardly direction. - While the foregoing is directed to embodiments of the present invention, other and further embodiments of the invention may be devised without departing from the basic scope thereof, and the scope thereof is determined by the claims that follow.
Claims (36)
1. An apparatus for dispensing a chemical reagent into a plating solution comprising:
a tank for containing the plating solution;
a vessel in fluid communication with the tank, wherein the vessel has an inlet and an outlet;
at least one horizontal shelf contained inside the vessel, wherein the at least one horizontal shelf is positioned to hold the chemical reagent and expose the chemical reagent to the plating solution flowing from the inlet to the outlet.
2. The apparatus of claim 1 , wherein at least one horizontal shelf is impermeable to the plating solution.
3. The apparatus of claim 1 , wherein the plating solution is an acidic, electrochemical anolyte and includes copper ions.
4. The apparatus of claim 3 , wherein a headspace is disposed above the at least one horizontal shelf.
5. The apparatus of claim 4 , wherein the headspace is in a range from about 5 cm to about 30 cm.
6. The apparatus of claim 5 , wherein the electrochemical anolyte flows from the inlet to the outlet via the headspace.
7. The apparatus of claim 6 , wherein the electrochemical anolyte is replenished by the chemical reagent.
8. The apparatus of claim 7 , wherein the chemical reagent comprises a copper source compound selected from the group consisting of copper hydroxide, copper carbonate, copper oxide, copper sulfate, copper phosphate and combinations thereof.
9. The apparatus of claim 1 , wherein the at least one horizontal shelf includes a flat shelf, a longitudinally grooved shelf, a tubular shelf or combinations thereof.
10. The apparatus of claim 9 , wherein the vessel comprises at least one porous material selected from the group consisting of a membrane, a filter, a frit, a mesh and combinations thereof.
11. An apparatus for dispersing a chemical reagent to a plating solution comprising:
a tank for containing the plating solution; and
a vertical vessel in fluid communication with the tank, comprising:
a lower portion of the vertical vessel including an inlet and an injector port;
an upper portion of the vertical vessel including an outlet and a manifold; and
the chemical reagent positioned between the inlet and the outlet.
12. The apparatus or claim 11 , wherein the lower portion expands radially outwardly.
13. The apparatus of claim 12 , wherein the injector port is positioned to direct the plating solution in a downward direction away from the output.
14. The apparatus of claim 11 , wherein the plating solution is an acidic, electrochemical anolyte and includes copper ions.
15. The apparatus of claim 11 , wherein a headspace is disposed above the chemical reagent.
16. The apparatus of claim 15 , wherein the headspace is in a range from about 5 cm to about 30 cm.
17. The apparatus of claim 16 , wherein the plating solution flows from the inlet to the outlet via the headspace.
18. The apparatus of claim 17 , wherein the plating solution is replenished by the chemical reagent.
19. The apparatus of claim 18 , wherein the chemical reagent comprises a copper source compound selected from the group consisting of copper hydroxide, copper carbonate, copper oxide, copper sulfate, copper phosphate and combinations thereof.
20. A method for replenishing copper in a plating solution comprising:
flowing the plating solution from a tank through an inlet of a vessel, wherein the vessel comprises a chemical reagent disposed on at least one shelf;
flowing the plating solution across the chemical reagent to enrich the plating solution with the chemical reagent; and
flowing the enriched plating solution from the vessel through an outlet to the tank.
21. The method of claim 20 , wherein at least one horizontal shelf is impermeable to the plating solution.
22. The method of claim 20 , wherein the plating solution has a pH in a range from about 2.0 to about 4.0
23. The method of claim 22 , wherein a copper concentration is monitored and controlled as a function of the pH.
24. The method of claim 20 , wherein the plating solution is an acidic, electrochemical anolyte and includes copper ions.
25. The method of claim 20 , wherein the plating solution flows through a headspace disposed above the at least one shelf.
26. The method of claim 25 , wherein the headspace is in a range from about 5 cm to about 30 cm.
27. The method of claim 26 , wherein the electrochemical anolyte flows from the inlet to the outlet via the headspace.
28. The method of claim 24 , wherein the chemical reagent comprises a copper source compound selected from the group consisting of copper hydroxide, copper carbonate, copper oxide, copper sulfate, copper phosphate and combinations thereof.
29. The method of claim 28 , wherein the at least one shelf includes a flat shelf, a longitudinally grooved shelf, a tubular shelf or combinations thereof.
30. The method of claim 29 , wherein the horizontal vessel comprises at least one porous material selected from the group consisting of a membrane, a filter, a frit, a mesh and combinations thereof.
31. A method for monitoring and controlling a pH setting of a plating solution in a tank comprising:
transferring an aliquot of the plating solution to a container;
pressurizing the container with a gas to transfer the aliquot to a vessel, wherein the vessel comprises an injector, a chemical reagent and a manifold;
passing the aliquot through the injector to enrich the aliquot with a portion of the chemical reagent;
transferring the enriched aliquot through the manifold to the plating solution in the tank;
determining a pH of the plating solution with a pH meter; and
comparing the pH to the pH setting and repeating the transferring of the enriched aliquot to the plating solution until the pH is equivalent to the pH setting.
32. The method of claim 31 , wherein a copper concentration is monitored and controlled as a function of the pH setting.
33. The method of claim 31 , wherein the pH setting is in a range from about 2.0 to about 4.0.
34. The method of claim 31 , wherein the plating solution is an acidic, electrochemical anolyte and includes copper ions.
35. The method of claim 31 , wherein the chemical reagent comprises a copper source compound selected from the group consisting of copper hydroxide, copper carbonate, copper oxide, copper sulfate, copper phosphate and combinations thereof.
36. An apparatus for dispensing a chemical reagent into a plating solution comprising:
a tank for containing the plating solution;
a vessel in fluid communication with the tank, wherein the vessel has an inlet and an outlet;
at least one impermeable shelf contained inside the vessel, wherein the at least one impermeable shelf is positioned to hold the chemical reagent and expose the chemical reagent to the plating solution flowing from the inlet to the outlet.